Silver Brazing Wire

Silver Brazing Wires Ag45

  • Silver brazing wires Ag45 Solidus 640 °C. Liquidus 680 °C. Forty degrees is the entire working interval of this filler. For anyone brazing a 0.8 mm stainless tube into a machined body, or joining copper to steel on an assembly that has already been finish-machined, that narrow band is the reason to specify Ag45 rather than a lower-silver grade: the filler becomes fluid quickly, fills by capillary action, and freezes again as soon as the torch or coil moves away.
  • INQUIRY

Ag45 silver brazing wire, silver brazing wires ag45

Silver Brazing Wire Ag45 (BAg45CuZnSn) is supplied as drawn wire in six standard diameters — 1.6, 2.0, 2.5, 3.2, 4.0 and 5.0 mm — on spools, in coils or as straightened cut lengths. Cut length, coil weight, spool type and carton marking are produced to order. This page is about the wire: the melt behaviour that decides your heat input, the drawing and winding controls behind consistent feed, and the joint types where the extra silver pays for itself.

Start With the Melt Band, Not the Silver Percentage

Buyers usually compare Ag25, Ag30 and Ag45 by silver content. The number that changes how a joint is actually made is the gap between solidus and liquidus:

  • Short interval, decisive freezing. With only 40 °C between first melt and full fluidity, the filler does not linger in a mushy state. Once heat is removed the joint sets, so the risk of filler running out of the joint or dropping through a vertical seam is lower than with wide-interval alloys.

  • Lower working temperature. Brazing is normally carried out around 650–710 °C, below the range where thin-wall stainless, cold-drawn copper tube and pre-machined surfaces begin to lose dimensional control.

  • Less heat-soak into the fixture and the part. Shorter time above working temperature means adjacent seals, elastomer seats, coatings and heat-treated zones see less thermal load — the practical reason Ag45 appears on assemblies that already contain non-metallic components.

  • Narrower capillary gap. Ag45 fills tight clearances well; joints are typically designed at 0.03–0.10 mm at brazing temperature. That makes it a fitter's alloy: the joint has to be machined or formed accurately, and the reward is a fillet that needs almost no dressing.

The trade-off is honest to state: higher silver content means higher metal cost per kilogram, and a narrow interval leaves less tolerance for poor fit-up or an unsteady flame. Ag45 is the wrong choice for rough, wide-gap joints on thick sections — a wider-interval, lower-silver filler handles those more economically.

Technical Data

Silver Brazing Wire Ag45 — Specification
PropertyValue
DesignationBAg45CuZnSn (GB/T 10046); equivalent to AWS A5.8 BAg-36 and EN 1044 AG104
CompositionAg 44.0–46.0 %, Cu 26.0–28.0 %, Zn 23.5–27.5 %, Sn 2.0–3.0 %, other ≤ 0.15 %
Solidus / liquidus640 °C / 680 °C
Working range650–710 °C (set to the joint, not to a single figure)
Standard diameters1.6 / 2.0 / 2.5 / 3.2 / 4.0 / 5.0 mm
FormsSpool · coil · straightened cut length · rolled preform rings
Joint clearance0.03–0.10 mm at brazing temperature
Base metalsCopper and copper alloys, carbon steel, stainless steel, nickel alloys; dissimilar pairs such as copper-to-stainless and steel-to-brass
FluxRequires silver brazing flux — the alloy contains no phosphorus and does not self-flux
CadmiumCadmium-free; Sn is used to depress melting rather than Cd

Four Process Controls That Decide How the Wire Behaves

Drawn silver filler is a small product with a short list of variables that actually matter. Ours are controlled at these four points, and each one maps to a problem you would otherwise meet at the bench:

Control pointWhat is heldWhat it prevents
Melt chemistrySilver, copper, zinc and tin charged in weighed sequence; each heat sampled and released against the BAg45CuZnSn window before casting continuesMelting range drifting between lots, so a proven brazing programme no longer works on a new delivery
Drawing scheduleReduction per pass and inter-pass annealing set for this alloy, not borrowed from a lower-silver gradeWork-hardened wire that kinks instead of bending, and surface cracking during forming
Diameter controlContinuous measurement during drawing; the mill certificate records the measured range for the lotFeed-rate variation on automatic stations, and coils that will not pass a fixed orifice
Winding tensionCross-wound spools at controlled tension; cut lengths roll-straightened before bundlingSnagging and bird-nesting on payoff, and cut pieces that curl out of the joint instead of lying in it

Two further steps are worth naming because they affect what you see on arrival: the wire is cleaned after the final pass so its surface is receptive to flux rather than carrying drawing lubricant, and every coil is sealed in a moisture barrier before cartoning, since a damp surface on silver filler is a direct route to porosity.

Forms and Packing

FormDetailWhere it fits
SpoolPlastic spools, layer-wound or cross-wound, weight per spool to your specificationMotorised feed, semi-automatic and indexing brazing stations
CoilTied coils in bagged units, diameters typically 1.6–3.2 mmBench work, field service, maintenance brazing
Cut lengthStraightened and cut to your dimension, bundled by count or by weightOperators who pre-place filler, and fixtures that locate a fixed length per joint
Preform ringRolled from the same wire to a stated ID/OD and wire diameterTube-in-socket and bore joints where filler volume must be repeatable

Cut length, spool weight, coil weight, carton printing and labels are all made to order, and mixed packs (for example a cut-length bundle plus the matching flux quantity per station) can be arranged. If several diameters are used on one line, tell us the consumption ratio and we will quote a combined packing that avoids half-used spools at month end.

Where the Extra Silver Is Justified

  • Thin-wall stainless and copper tube. Wall sections under about 1 mm lose strength and roundness quickly under prolonged heat. The 640–680 °C band shortens the exposure window.

  • Dissimilar-metal joints. Copper to stainless, steel to brass, and joints between materials with different expansion rates: the higher-silver filler has more capacity to accommodate the strain that develops on cooling.

  • Assemblies with heat-sensitive neighbours. Brazing close to O-ring grooves, polymer seats, painted or plated surfaces, or already-finished bores where scale and distortion would mean rework.

  • Instrument, sensor and manifold bodies. Small joints with tight clearance and a visible fillet, where a narrow melt band and a low working temperature keep the part within tolerance.

  • Electrical contacts and conductor joints. Where the joint is expected to carry current and resist thermal cycling, and where overheating the copper would soften it.

  • Induction and resistance brazing. A defined set point and short dwell suit coil-based heating, provided the wire diameter is consistent from lot to lot.

Ag25 or Ag45: Choosing on Joint Duty, Not on Price per Kilo

Joint conditionAg25 (BAg25CuZnSn)Ag45 (BAg45CuZnSn)
Melt band680–760 °C, wide pasty interval640–680 °C, narrow interval
Fit-up toleranceForgiving; fills wider and uneven gapsRequires accurate fit; designed for 0.03–0.10 mm
Thin-wall partsUsable with heat controlBetter suited; shorter exposure above working temperature
Fillet appearanceFuller fillet, more dressing on visible jointsTight, low fillet needing little finishing
Metal cost per kgLowerHigher
Typical useHigh-volume tube joints, general fabrication, repairThin-wall, dissimilar, heat-sensitive and precision assemblies

Many plants keep both on the shelf and let the drawing decide. If you are unsure which side of the line a particular joint falls on, send the joint detail — wall thickness, materials, clearance and what sits nearby — and we will give a reasoned recommendation rather than defaulting to the higher-silver option.

Bench Notes for Ag45

  • Fit matters more than flux. At 0.03–0.10 mm clearance the filler is drawn in by capillary action; at 0.3 mm it will bridge but not penetrate, and the joint will look filled while leaking.

  • Heat the heavier part first. On dissimilar joints, bring the higher-mass or lower-conductivity component up to temperature and let conduction carry heat across the gap. Applying the torch to the thin side is the usual cause of a burnt edge and an unfilled root.

  • Do not over-flux. A thin, even coating on both faces is enough. Excess flux boils, traps gas and leaves inclusions that appear as porosity after cleaning.

  • Feed at the seam, not into the flame. Touch the wire to the joint edge and let the part melt it. Wire held in the flame oxidises before it reaches the gap.

  • Clean while warm. Flux residue from silver brazing is glassy and hard once cold; soaking in warm water immediately after the part is handleable removes it with far less mechanical work.

Frequently Asked Questions

Why does Ag45 wire cost more per kilogram than Ag25 wire?

Silver is the dominant cost in the alloy and the silver share is nearly double, so cost per kilogram is higher — that part is arithmetic. Cost per finished joint is a different calculation: filler consumed per joint, rework rate, and any straightening or re-machining needed after distortion. On thin-wall or heat-sensitive parts the lower working temperature can remove a finishing operation, which offsets part of the filler price. We are happy to work through that comparison on your actual joint.

What is the difference between Ag45 brazing wire and Ag45 rod?

Same alloy, different delivery. Wire comes as continuous drawn lengths (spool, coil) or straightened cut pieces, so filler can be fed continuously or pre-placed; rod comes as straight sticks fed by hand at the joint. If a fixture or feeder positions the filler for you, wire is the practical form.

Can Ag45 wire braze stainless without annealing the part?

It reduces the exposure, it does not remove it. Every brazing operation puts heat into the part; what the narrow 640–680 °C band buys you is a shorter time above the temperature where work-hardened stainless or cold-drawn copper starts to soften. Wall thickness, heat source and dwell still decide whether the part holds tolerance.

Is Ag45 suitable for induction brazing?

Yes, and the short interval is an advantage there: the coil can be set to a defined temperature and the joint filled in a brief dwell. The requirement is consistent filler cross-section, because fixtures and coil geometry are usually built around one wire diameter.

Do you supply Ag45 preforms as well as straight wire?

Yes — rings and simple shaped preforms rolled from the same wire, to a stated inner diameter, outer diameter and wire size. Preforms are useful when filler volume per joint has to be identical across a shift.

What do you need in order to quote?

Diameter and form, cut length or spool weight if you have a preference, base metals and joint type, monthly or annual quantity, and any packing or marking requirement. Send those and you will receive price, lead time and a certificate of analysis sample in return.

Ask for an Ag45 Wire Quotation

Tell us the diameter, the form you want the wire in, and the quantity per order — we will confirm price, lead time and the documentation supplied with each lot. Trial lengths for brazing on your own fixture can be arranged before you commit to a production quantity.

PREVIOUS: No record! NEXT: Silver Brazing Wires Ag50